Grano Colour


Grano Colour application method continued

Grano Colour application method

Expansion joints must be cut before application commences

Sweep the floor to remove all dust and debris

Dampen the surface of the base concrete

Apply Grano Colour by dry-shake method at a rate of 5kg/m2 directly to the surface of the entire screed

Leave to soak up the water from the screed

Wood float the Grano Colour into the surface

Combine 3 volumes of water and 1 volume of hydrochloric acid in a plastic bucket and apply this solution liberally to the base concrete

Wire-brush the surface vigorously and then allow the acid solution to react for a further 15 minutes

Flush clean with water and remove all loose material using a hard bristle broom

Steel float immediately to obtain a smooth finish

To obtain a smoother surface, sift Grano Colour through a very fine sieve or stocking to remove all coarse material and apply to the wet surface

Steel float immediately to a very smooth finish Leave the completed floor to dry for 24 hours

Curing Wet the surface 3 times daily for a minimum of 6 days. Allow to dry for a minimum of 8 days before sealing.

Sealing When properly cured and dry, the finished work must be sealed using an appropriate sealer. See data sheet overleaf.

Grano Colour colour chart

Underfloor heating should be installed at this point

Add water to obtain a stiff consistency

Combine 4 volumes of crusher dust or clean river sand with 1 volume of 42.5 cement

Note the consistency

Mix thoroughly

Mix equal volumes of plaster sand and OPC. Add Weber Key-it to create a creamy, brushable slurry. Apply to the base concrete using a block-brush

bamboo

brown

charcoal

chocolate

clay

green

grey

pebble

These colour representations are as accurate as the printing process permits. It is advisable to view an actual product sample before a final choice is made.

terracotta Place the screed to a minimum thickness of 30mm and compact thoroughly The placing of the screed should take place while the slurry coat is wet

Strike level

Wood float the surface DO NOT add extra water during this process

photographed with the kind co-operation of Denise Suttie

Saint-Gobain Construction Products SA (Pty) Ltd 77 Ostend Road, Germiston South, Johannesburg Tel.: +27 11 345-5300 Fax: +27 11 345-5301 Sales : 0860 27 28 29 or visit www.weber-tylon.co.za

white

To the best of our knowledge and belief, this information is true and accurate. As the conditions of use and any labour involved are beyond our control, the end-user must satisfy himself by prior testing that the product is suitable for his specific application. Products are sold subject to our Standard Conditions of Sale.


Grano Colour data sheet About this product

Features and benefits

Grano Colour is a cement-based, integrally coloured granolithic product for the surface hardening of freshly placed concrete or screeds.

• • • • • • • • •

Applied by dry-shake method, it may be steel floated to a smooth finish or imprinted to obtain tiled or paved effects. For interior or exterior use.

Technical data Abrasion strength*

<3.2cm3/50cm2 TS:699/DIN:52108 (Method of Böhme)

*Value obtained in laboratory conditions.

Carefully graded aggregates to produce a fine finish Improved abrasive resistance Colours concrete or screed to a depth of about 2mm No risk of colour being rubbed off or abraded Colours are UV stable Quality assured raw materials Exceptional and consistent quality Backed by superior technical support Available in a range of colours

Technical services

Storage and shelf life

Weber has a team of experienced advisors available to provide technical support. Technical helpline : 0860 27 28 29 or visit www.weber-tylon.co.za Contact the C&CI library (www.cnci.org.za) for technical information on cement and concrete.

When stored, unopened in a dry place at temperatures above 50C, shelf life is 12 months from date of manufacture.

Use To provide a very hard-wearing, attractive colouring system for the surface of concrete or screeds.

Suitable surfaces Freshly placed concrete or screeds. Grano Colour is floated into the surface of the wet screed or concrete. Grano Colour screed (minimum 25mm)

Grano Colour

steel re-inforced concrete

steel re-inforced concrete

compacted soil

compacted soil

Good practice Do not apply : • if frost is forecast within 4 hours of use • in temperatures below 50C or above 300C • on elevations in direct sunlight or where the substrate is hot Work should be completed in a sequence that will enable a wet edge to be maintained across the entire floor and thus prevent dry joints Cover during hot/dry weather to avoid premature drying To ensure colour consistency, the required material should be of the same batch number.

Specifying “Apply Weber Grano Colour at a rate of 5kg/m2 in accordance with the manufacturer’s instructions.”

Packaging and coverage Grano Colour is supplied in 20kg paper bags. Coverage is approximately 3 to 4m2 per bag.

Safety instructions Contains cement, which is alkaline when wet and can cause skin irritation. Use eye protection and gloves and avoid prolonged skin contact. Avoid inhalation of dust. Wash skin contamination away with warm soapy water. Remove splashes to the eyes by prolonged irrigation and consult a doctor. Do not ingest.

Surface preparation Remove all bleed water.

Masking Mask all areas where there is a risk of splashing and staining and where straight edges are required.

Mixing No mixing required. Dust Grano Colour in dry powder form onto the surface of the concrete or screed before final wood- and steel floating takes place. See application method.

Laying a screed Preparing the substrate

Applying the slurry coat

• • • • •

•M ix equal volumes of plaster sand and OPC and add Weber Key-it to create a creamy, brushable consistency. • A pply this slurry to the base concrete using a block-brush or broom. • T he placing of the screed should take place while the slurry coat is wet.

Dampen the surface of the base concrete. Combine 3 volumes of water and 1 volume of hydrochloric acid in a plastic bucket. Apply this solution liberally to the base concrete. Wire-brush the surface vigorously. Allow to react for a further 15 minutes. Flush clean with water and remove all loose material using a hard bristle broom.

Mixing the screed • • • • •

Combine 4 volumes of crusher dust or clean river sand with 1 volume of 42.5 cement. Add water to obtain a stiff consistency. Place the screed to a minimum thickness of 30mm. Compact thoroughly and strike level. Wood float the surface. Do not add extra water during this process.

Application The surface must be damp, but not glistening with water. ▲ Apply Grano Colour by dry-shake method at a rate of 5kg/m2 directly to the surface of the entire screed. ▲ Leave to soak up the water from the screed. ▲ Wood float the Grano Colour into the surface. ▲ Steel float immediately to obtain a smooth finish. ▲ To obtain a smoother surface, sift Grano Colour through a very fine sieve or stocking to remove all coarse material. Apply this sifted material to the wet surface and steel float. ▲ Leave the completed floor to dry for 24 hours.

Curing Wet the surface 3 times daily for a minimum of 6 days. Allow to dry for a minimum of 8 days before sealing.

Sealing When properly cured and dry, the finished work must be sealed using an appropriate sealer in accordance with its data sheet. Please contact our Technical helpline on 0860 27 28 29 for information on the range of Weber sealers and sealing methods. Please note : If a floor is sealed before it is properly dry, white marks will appear on the surface. This is as a result of the salts migrating to the surface and being trapped under the sealer. This can only be rectified by stripping the sealer and sanding the surface. The floor must then be cleaned and re-sealed. It is therefore clear that it is better to wait for the floor to dry properly before sealing. An easy test to determine whether a floor is dry enough to seal : ■ Place a piece of dense plastic flat on the floor. ■ Leave overnight. ■ If any moisture has collected on the bottom of the plastic, the floor should be left to dry for at least 2 days before re-testing.